1.KimiaCoposisi
Bahan | Komposisi kimiawi (%) | ||||
Ni | Cr | Si | Mn | Al | |
KP (Chromel) | 90 | 10 | |||
KN (Alumel) | 95 | 1-2 | 0,5-1,5 | 1-1.5 |
2.sipat fisikjeung sipat Mékanis
Bahan | Kapadetan (g/cm3) | titik lebur ℃) | Kakuatan regangan (Mpa) | Résistansi volume (μΩ.cm) | Laju elongasi (%) |
KP (Chromel) | 8.5 | 1427 | >490 | 70,6 (20 ℃) | > 10 |
KN (Alumel) | 8.6 | 1399 | >390 | 29.4(20℃) | > 15 |
3.rentang Niley EMF dina suhu béda
Bahan | Nilai EMF Vs Pt(μV) | |||||
100 ℃ | 200 ℃ | 300 ℃ | 400 ℃ | 500 ℃ | 600 ℃ | |
KP (Chromel) | 2816~2896 | 5938~6018 | 9298~9378 | 12729~12821 | 16156~16266 | 19532~19676 |
KN (Alumel) | 1218~1262 | 2140~2180 | 2849~2893 | 3600~3644 | 4403~4463 | 5271~5331 |
Nilai EMF Vs Pt(μV) | ||||
700 ℃ | 800 ℃ | 900 ℃ | 1000 ℃ | 1100 ℃ |
22845~22999 | 26064~26246 | 29223~29411 | 32313~32525 | 35336~35548 |
6167~6247 | 7080~7160 | 7959~8059 | 8807~8907 | 9617~9737 |
TIPE K (CHROMEL vs ALUMEL )dipaké dina atmosfir pangoksidasi, inert atawa pangréduksi garing. Paparan vakum dugi ka période waktos pondok. Kedah ditangtayungan tina atmosfir sulfur sareng pangoksidasi marginal. Dipercaya sareng akurat dina suhu anu luhur.
150 0000 2421